Engineering Procedure SAEP-352 Welding Procedures Review and Approval
20 October 2009
Welding Standards Committee Members Awwami, Adnan Ni'Mah, Chairman Rao, Sanyasi, Vice Chairman Carrera, R L Carswell, Raymond J. Juraifani, Hatim Hamad Keen, Peter David Muslim, Husain Muhammad Nasri, Nadhir Ibrahim Niemeyer, Dennis Charles Sabti, Tareq Ibrahim Sayed Nasir, Ghalib Taher
Saudi Aramco DeskTop Standards Table of Contents 1 2 3 4 5
Scope............................................................. 2 Conflicts and Deviations................................. 2 Applicable Documents.................................... 2 Definitions and Acronyms............................... 6 Instructions and Approval Responsibility........ 7
Table 1 – Welding Procedure Technical Approval Responsibility………..……….. 9 Appendix I – Welding Master Set Preparation and Approval..................... 12 Appendix II – Welding Package Review and Approval Process for Company Projects................................ 13 Appendix III – Welding Package Review and Approval Process for Repair/Maintenance/Alterations............ 14
Previous Issue: 31 May 2003
Next Planned Update: 20 October 2014 Page 1 of 14
Primary contact: Al-Sabti Tareq Ibrahim on 966-3-8760236 Copyright©Saudi Aramco 2009. All rights reserved.
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
1
2
SAEP-352 Welding Procedures Review and Approval
Scope 1.1
This procedure specifies the responsibilities for welding procedure review and approval. This procedure applies to pressure vessels, process equipment or components, piping, pipelines, and structures fabricated to a variety of standards, such as but not limited to ASME SEC I, IV, VIII, B31.1, B31.3, B31.4, B31.8 and API STD 560, 620 and 650, and AWS D1.1.
1.2
Additional requirements may be contained in Scopes of Work, Drawings, or other Instructions or Specifications pertaining to specific items of work.
Conflicts and Deviations Conflicts between this Engineering Procedure and any other Saudi Aramco Standard shall be resolved by the Consulting Services Department in writing.
3
Applicable Documents Unless stated otherwise, all Standards, Specifications, and Codes referenced in this procedure shall be of the latest issue (including revisions, addenda, and supplements) and are considered a part of this procedure. 3.1
Saudi Aramco References Saudi Aramco Engineering Procedure SAEP-310
Piping and Pipeline Repair
Saudi Aramco Engineering Standards SAES-D-008
Repairs, Alterations, and Rerating of Pressured Equipment
SAES-D-108
Storage Tank Integrity
SAES-D-116
Underground Storage Tank System
SAES-K-001
Heating, Ventilating and Air Conditioning (HVAC)
SAES-L-350
Construction Requirements for Metallic Plant Piping
SAES-L-450
Construction Requirements for Cross-Country Pipelines
SAES-L-460
Pipelines Crossing Under Roads and Railroads
SAES-L-850
Design of Submarine Pipelines and Risers Page 2 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
SAEP-352 Welding Procedures Review and Approval
SAES-M-001
Structural Design Criteria for Non-Building Structures
SAES-M-005
Design and Construction of Fixed Offshore Platforms
SAES-M-009
Design Criteria for Blast Resistant Buildings
SAES-T-744
Design Criteria/Installation of Communication Towers
SAES-W-010
Welding Requirements for Pressure Vessels
SAES-W-011
Welding Requirements for On-Plot Piping
SAES-W-012
Welding Requirements for Pipelines
SAES-W-013
Welding Requirements for Offshore Structures
SAES-W-014
Weld Overlays and Welding of Clad Materials
SAES-W-015
Strip Lining Application
SAES-W-016
Welding of Special Corrosion-Resistant Materials
SAES-W-017
Welding Requirements for API Tanks
Saudi Aramco Materials System Specifications 01-SAMSS-010
Fabricated Carbon Steel Piping
01-SAMSS-017
Auxiliary Piping for Mechanical Equipment
01-SAMSS-035
API Line Pipe
01-SAMSS-038
Small Direct Charge Purchases of Pipe
01-SAMSS-046
Stainless Steel Pipe
01-SAMSS-333
High Frequency Welded Line Pipe
02-SAMSS-001
Piping Components for Low Temperature Services
02-SAMSS-005
Butt Welding Pipe Fittings
02-SAMSS-006
Hot Tap and Stopple Fittings
02-SAMSS-008
Insulating Joints/Spools for Cathodic Protection
02-SAMSS-009
Design and Fabrication of Scraper Traps
02-SAMSS-010
Flanged Insulating Joints/Spools for Cathodic Protection
02-SAMSS-011
Forged Steel Weld Neck Flanges for Low, Intermediate and High Temperature Service
04-SAMSS-035
General Requirements for Valves Page 3 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
SAEP-352 Welding Procedures Review and Approval
04-SAMSS-053
Steel Lubricated Plug Valves - Flanged and Welding End
12-SAMSS-007
Fabrication of Structural and Miscellaneous Steel
12-SAMSS-014
Pre-Engineered Metal Building
27-SAMSS-001
Packaged Water Cooled Centrifugal Chillers for Utility Services
27-SAMSS-002
Direct Expansion Air Conditioning Systems for Offshore Facilities
27-SAMSS-003
Manufacture of Non-Industrial Cooling Towers
30-SAMSS-001
Diesel Engines
31-SAMSS-001
Centrifugal Compressor
31-SAMSS-002
Packaged Reciprocating Plant and Instrument Air Compressors
31-SAMSS-003
Reciprocating Compressors for Process Air or Gas Service
31-SAMSS-004
Centrifugal Pumps
31-SAMSS-005
Centrifugal Fluorocarbon Refrigeration Units for Industrial/Process Services
31-SAMSS-006
Packaged, Integrally Geared Centrifugal Air Compressors
31-SAMSS-009
Positive Displacement Pumps - Controlled Volume
31-SAMSS-010
Submersible Pumps and Motors for Water Well and Offshore Service
31-SAMSS-012
Shaft Sealing Systems for Centrifugal and Rotary Pumps
32-SAMSS-001
Special Purpose Steam Turbines for Generator Sets
32-SAMSS-004
Manufacture of Pressure Vessels
32-SAMSS-005
Manufacture of Atmospheric Tanks
32-SAMSS-006
Manufacture of Low Pressure Tanks
32-SAMSS-007
Manufacture of Shell and Tube Heat Exchangers
32-SAMSS-008
Inlet Air Filtration Systems for Combustion Gas Turbines
32-SAMSS-009
General Purpose Steam Turbines
32-SAMSS-010
Special Purpose Steam Turbines Page 4 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
3.2
SAEP-352 Welding Procedures Review and Approval
32-SAMSS-011
Manufacture of Air-cooled Heat Exchangers
32-SAMSS-013
Lubrication, Shaft Sealing and Control Oil Systems
32-SAMSS-016
Inlet Air Filtration Systems for Centrifugal Air Compressors
32-SAMSS-017
Side-Entry Mixers
32-SAMSS-019
Manufacture of Plate and Frame Heat Exchangers
32-SAMSS-020
Manufacture of Trays and Packing
32-SAMSS-021
Manufacture of Industrial Boilers
32-SAMSS-022
Manufacture of Components for Flare Systems
32-SAMSS-027
Manufacture of Electric Heat Exchangers
32-SAMSS-028
Manufacture of Double Pipe Heat Exchangers
32-SAMSS-029
Manufacture of Fire Heaters
32-SAMSS-030
Manufacture of Small Tanks
32-SAMSS-031
Manufacture of Clad Vessels and Exchangers
32-SAMSS-033
Reverse Osmosis Systems
32-SAMSS-035
Manufacture of Heat Recovery Steam Generator
32-SAMSS-036
Manufacture of Small Pressure Vessels
32-SAMSS-100
Combustion Gas Turbines
34-SAMSS-611
Safety Relief Valves Conventional and Balanced Types
34-SAMSS-612
Safety Relief Valves Pilot Operated Types
34-SAMSS-711
Control Valves
45-SAMSS-005
Valves and Wellhead Equipment Requirements per API SPEC 6A
Industry Codes and Standards American Petroleum Institute API STD 560
Fired Heaters for General Refinery Services
API STD 620
Design and Construction of Large, Welded, LowPressure Storage Tanks
API STD 650
Welded Steel Tanks for Oil Storage
API STD 1104
Welding of Pipelines and Related Facilities Page 5 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
SAEP-352 Welding Procedures Review and Approval
American Society of Mechanical Engineers ASME B31.1
Power Piping
ASME B31.3
Process Piping
ASME B31.4
Pipeline Transportation Systems for Liquid Hydrocarbons and other Liquids
ASME B31.8
Gas Transmission and Distribution Piping Systems
ASME SEC I
Rules for Construction of Power Boilers
ASME SEC IV
Rules for Construction of Heating Boilers
ASME SEC VIII
Rules for Construction of Pressure Vessels
ASME SEC IX
Welding and Brazing Qualifications
American Welding Society AWS D1.1 4
Structural Welding Code-Steel
Definitions and Acronyms Application Approval: Approval acquired from Inspection Department to apply technically approved welding procedure. ID generally verifies that the intended application of previously approved welding procedures is within the welding procedure's variables (e.g., diameter, thickness, materials, service, etc.) approval range. CSD: Consulting Services Department Welding Specialist/Engineer or CSD's Appointed Representative (e.g., Aramco Services Company Welding Specialist/Engineer). ID: Inspection Department Vendor, Operations or Project Inspector or Inspection Representative. PMC: A Program Management Contractor. SAPMT: Saudi Aramco Project Management Team or someone acting on their behalf such as PMC. PMT Designated Welding Representative (PMT DWR): A welding engineer / inspector assigned to and contracted by SAPMT who has the approval authority for project(s) associated welding procedures. PQR: Performance Qualification Record
Page 6 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
SAEP-352 Welding Procedures Review and Approval
Technical Approval: Approval of welding procedures acquired from CSD or PMT Designated Welding Representative. This approval indicates that the welding procedure was qualified to Saudi Aramco and/or industry standards or codes and it is acceptable for the intended application. Every page of the welding procedure specifications should include the reviewer signature and/or approval stamp. Weld and Line Designation Table: A table that lists the applicable welding procedures, approval conditions (e.g., low temperature, sour service, etc.), welding process, and any general welding information pertinent to those applicable welding procedures. Weld Map: A schematic one line diagram of pressure containing equipment (e.g., pressure vessel or tank). The map should indicate where each approved welding procedure will be applied. Welding Master Set (WMS): It is compilation of welding procedures prepared by vendor/fabricator. It is a standardized set of welding procedures that is used with a generic Weld and Line Designation Table and/or generic Weld Map, which include the material and service application information. WP: Welding Package. WPS: Welding Procedure Specifications. 5
Instructions and Approval Responsibility 5.1
CSD shall be the technical approval authority for the followings: a)
All Saudi Aramco Project welding procedures for applications listed in Table 1 from either in-kingdom or out of kingdom fabricators and construction contractors. Appendix II is a flowchart that indicates the review process for Saudi Aramco projects.
b)
"Welding Master Set" submissions for the applications listed in Table 1 from in-Kingdom and Gulf Cooperation Council fabricators. See Appendix I for details on welding master set's preparation and approval. Appendix II is a flowchart that indicates the review process for Saudi Aramco projects. The Welding Master Set (WMS) is submitted to PMT for CSD's one-time technical approval. When WMS is approved by CSD then it can be often used in various Saudi Aramco projects if ID approves the application.
c)
Maintenance/repair/alteration applications. Appendix III is a flow chart that indicates the review process.
Page 7 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
5.2
SAEP-352 Welding Procedures Review and Approval
A PMT designated welding representative assigned to and contracted by SAPMT may be the approval authority for project(s) associated welding procedures. He must review the welding procedures for all applications listed in Table 1, and as requested by PMT CSD will interview and approve the PMT designated welding representative. Written examinations may be requested and prepared by CSD, this will depend on the project scope. With coordination with SAPMT, CSD will periodically audit some of his welding procedures review.
5.3
For applications not listed or not requiring CSD/PMT DWR review in Table 1 the qualified welding procedures shall be available at the fabrication/welding site (e.g., vendor shop, field fabrication, etc.) for review by the Inspector, if requested. The procedures shall be included in the project or shop documentation record books.
5.4
If the welding procedure is approved to the latest edition of the welding standards, then the fabricator/construction contractor is permitted to use the welding procedure without CSD/PMT DWR review. The assigned inspector must verify that the qualification range (e.g., diameter, thickness, material grade, etc.) of the welding procedure is still applicable to the new work.
5.5
If the welding procedure is approved to a previous edition of the welding standards, then fabricator/construction contractor is permitted to use it, if it was not affected by the revisions. The fabricator/construction contractor must write a formal letter to PMT or Engineering/Maintenance Div. indicating that the subject welding procedure still complies with the latest edition of Saudi Aramco Welding Standards. The assigned inspector must verify that the qualification range (e.g., diameter, thickness, material grade, etc.) of the welding procedure is still applicable to the new work.
5.6
If the previously approved welding procedure is invalidated by a change in the welding standard, a revised welding procedure, along with the old approved copy, must be submitted for CSD/PMT DWR review. The assigned inspector must verify that the qualification range (e.g., diameter, thickness, material grade, etc.) of the welding procedure is still applicable to the new work.
20 October 2009
Revision Summary Major revision.
Page 8 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
SAEP-352 Welding Procedures Review and Approval
Table 1 – Welding Procedure Technical Approval Responsibility Component Boiler
Compressor
Fired Heater
Fitting Piping Pipeline
Flare System
Application
Specification
Welding Standard
Review/Approval Responsibility CSD/PMT DWR
Not Required (1)
Manufacture of Boilers Repairs, Alterations, and Re-rating Axial , Centrifugal, & Expander Compressors Packaged Reciprocating Plant & Instrument Air Compressor Reciprocating Compressor Packaged, Integrally Geared Centrifugal Air Compressor Inlet Air Filtration Systems for Centrifugal Air Compressor Coils Only Repairs, Alterations, and Re-rating
32-SAMSS-021 SAES-D-008
SAES-W-010 SAES-W-010
31-SAMSS-001
NA
X
31-SAMSS-002
NA
X
31-SAMSS-003
NA
X
31-SAMSS-006
NA
X
32-SAMSS-016
NA
X
32-SAMSS-029 SAES-D-008
X X
Fabricated Carbon Steel Piping
01-SAMSS-010
High Frequency Welded Pipe
01-SAMSS-333
Scraper Traps
02-SAMSS-009
Construction of Plant Piping
SAES-L-350
Construction of Pipelines Pipeline Crossings Under Roads and Railroads Submarine Pipelines and Risers
SAES-L-450
SAES-W-011 SAES-W-010 SAES-W-011 SAES-W-012 01-SAMSS-333 SAES-W-011 SAES-W-012 SAES-W-011 SAES-W-016 SAES-W-012
SAES-L-460
SAES-W-012
X
SAES-L-850 SAEP-310
SAES-W-012 SAES-W-011 SAES-W-012 SAES-W-011 NA NA
X
Piping and Pipeline Repair Spectacle Blinds Auxiliary Piping Mounted Skids Procurement & Manufacturing of Line Pipe (large quantity) Procurement & Manufacturing of Line Pipe (small quantity) Manufacturing of Stainless Steel Pipe Manufacturing of Piping Components for Low Temperature Service Manufacturing of Butt Welding Pipe Fittings Manufacturing of Hot Tap and Stopple Fittings Manufacturing of Insulating Joints/Spools for Cathodic Protection Manufacturing of Flanged Insulating Joints/Spools for Cathodic Protection Manufacture of Components for Flare Systems
01-SAMSS-017
X X
X X X X X
X X X X
01-SAMSS-035
NA
X
01-SAMSS-038
NA
X
01-SAMSS-046
NA
X
02-SAMSS-001
NA
X
02-SAMSS-005
NA
X
02-SAMSS-006
NA
X
02-SAMSS-008
NA
X
02-SAMSS-010
NA
X
32-SAMSS-022
NA
X
Page 9 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
SAEP-352 Welding Procedures Review and Approval
Table 1 – Welding Procedure Technical Approval Responsibility (cont'd) Component
Heat Exchanger
Heat Recovery Steam Generator
Miscellaneous
Pump
Structural steel
Tank
Application
Specification
Shell and Tube Heat Exchanger Air-Cooled Heat Exchanger Plate and Frame Heat Exchanger Electric Heat Exchanger Double Pipe Heat Exchanger Clad Heat Exchanger
32-SAMSS-007 32-SAMSS-011 32-SAMSS-019 32-SAMSS-027 32-SAMSS-028 32-SAMSS-031
Repairs, Alterations, and Re-rating
SAES-D-008
Manufacture of Heat Recovery Steam Generators Brazing Centrifugal Fluorocarbon Refrigeration Units for Industrial/Process Services Diesel Engines Direct Expansion Air Conditioning Systems for Offshore Facilities Heating, Ventilating and Air Conditioning (HVAC) Lubrication, Shaft Sealing and Control Oil Systems Manufacture of Non-Industrial Cooling Towers Packaged Water Cooled Centrifugal Chillers for Utility Services Reverse Osmosis System Side-Entry Mixers Centrifugal Pump Positive Displacement Pump Submersible Pump Shaft Sealing System Construction of Fixed Offshore Platforms Fabrication of Structural and Miscellaneous Steel Pre-Engineered Metal Buildings Non-Building Structures Blast Resistant Buildings Communication Towers Atmospheric Tank Low Pressure Tank Small Tank Repair, Alteration, and Reconstruction Underground Storage Tank
Welding Standard
Review/Approval Responsibility CSD/PMT DWR
Not Required (1)
SAES-W-010 SAES-W-010 SAES-W-010 SAES-W-010 SAES-W-010 SAES-W-010 SAES-W-010 SAES-W-014 SAES-W-015
X X X X X X
32-SAMSS-035
SAES-W-010
X
NA
NA
X
31-SAMSS-005
NA
X
30-SAMSS-001
NA
X
27-SAMSS-002
NA
X
SAES-K-001
NA
X
32-SAMSS-013
NA
X
27-SAMSS-003
NA
X
27-SAMSS-001
NA
X
32-SAMSS-033 32-SAMSS-017 31-SAMSS-004 31-SAMSS-009 31-SAMSS-010 31-SAMSS-012
NA NA NA NA NA NA
X X X X X X
SAES-M-005
SAES-W-013
12-SAMSS-007
NA
X
12-SAMSS-014 SAES-M-001 SAES-M-009 SAES-T-744 32-SAMSS-005 32-SAMSS-006 32-SAMSS-030
NA NA NA NA SAES-W-017 SAES-W-017 SAES-W-017
X X X X X X X
SAES-D-108
SAES-W-017
X
SAES-D-116
SAES-W-017
X
X
X
Page 10 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
SAEP-352 Welding Procedures Review and Approval
Table 1 – Welding Procedure Technical Approval Responsibility (cont'd) Component
Turbine
Valve
Application
Specification
Welding Standard
Review/Approval Responsibility CSD/PMT DWR
Not Required (1)
Special Purpose Steam Turbine Inlet Air Filtration System for CGT General Purpose Steam Turbine Special Purpose Steam Turbine Combustion Gas Turbine General Requirement Steel Lubricated Plug Valve Safety Relief Valve Conventional and Balanced Types Safety Relief Valve Pilot Operated Types Control Valve Valve and Wellhead Equipment per API SPEC 6A Manufacture of Pressure Vessel Manufacture of Small Pressure Vessel Manufacture of Clad Vessel
32-SAMSS-001 32-SAMSS-008 32-SAMSS-009 32-SAMSS-010 32-SAMSS-100 04-SAMSS-035 04-SAMSS-053
NA NA NA NA NA NA NA
X X X X X X X
34-SAMSS-611
NA
X
34-SAMSS-612
NA
X
34-SAMSS-711
NA
X
45-SAMSS-005
NA
X
32-SAMSS-004 32-SAMSS-036 32-SAMSS-031
Repairs, Alterations, and Re-rating
SAES-D-008
Manufacture of Trays and Packing
32-SAMSS-020
SAES-W-010 SAES-W-010 SAES-W-010 SAES-W-010 SAES-W-014 SAES-W-015 NA
Vessel
X X X X X
Notes: 1.
Formal approval is not required. However, all WPS/PQR/Weld Map documents must be available for the inspector review or verification upon his request.
2.
In special cases the PMT or the Engineering/Maintenance Division may request CSD procedure review for any application. This may be done even though procedure review is not required according to Table 1 or is not listed in Table 1.
Page 11 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
SAEP-352 Welding Procedures Review and Approval
Appendix I – Welding Master Set Preparation and Approval 1.
Each fabricator/vendor awarded a contract or purchase order will compile all CSD revised previously approved welding procedures and any welding procedures, intended to be used in Saudi Aramco projects.
2.
Revised previously approved welding procedures must be submitted in new forms, unsigned, and the approved copy is attached to compare welding parameters between the two copies.
3.
The master set must include typical "Weld Maps", "Weld Description" sheet, "Request for Welding Procedure Approval" form and any supporting document required to be submitted by Saudi Aramco Welding Standard (SAES-W-010, SAES-W-011, etc.). It is recommended that a distinct identification system is used for the WPS and the revision number (e.g., WPS # is WMS P1-P8-1 and the revision # is M0, here both WMS and M indicate that the welding procedure is part of welding master set).
4.
The PQRs must be either the originals, certified/stamped copies, or colored copies of the originals. The qualification tests must be performed by independent testing agency approved by Saudi Aramco (Contact CSD Welding Group to get the updated list of the approved independent test agencies).
5.
The time required to review each master set will depend on the number of the submitted welding procedures and the pertinent technical welding requirements (e.g., PWHT, hardness test, impact toughness test, etc.). The table below lists the estimated time to review welding master sets. Estimated Time to Review Welding Master Sets Number of MS Welding Procedure
Time to Complete Review
Up to 50
6 Weeks
>50 to 100
10 Weeks
> 100
16 Weeks
6.
After the initial technical approval, the welding procedures can be applied in various company projects if ID approves the application.
7.
The fabricator/ Construction Contractor must continuously review the approved welding procedures to ensure their conformance with the latest applicable Saudi Aramco Welding Standards and Industry Codes.
Page 12 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
SAEP-352 Welding Procedures Review and Approval
Appendix II – Welding Package Review and Approval Process for Company Projects Fabricator/Construction Contractor prepares WP complying Saudi Aramco Welding Engineering Standards
PMT screens WP:
Fabricator/Construction Contractor receive and review CSD/PMT DWR comments and correct WP deficiencies
WP rejected
Is it IK/GCC fabricator’s WMS? OR Does it need CSD/PMT DWR formal approval as per Table 1?
No
Yes CSD welding specialist/engineer or PMT DWR reviews WP
PMT receives WP review Results WP accepted
WP rejected
ID reviews and approves the application of WP WP accepted PMT formally accepts the WP and sends the approval to Fabricator/Construction Contractor
Fabricator/Construction Contractor can use the welding procedure
Page 13 of 14
Document Responsibility: Welding Standards Committee Issue Date: 20 October 2009 Next Planned Update: 20 October 2014
SAEP-352 Welding Procedures Review and Approval
Appendix III – Welding Package Review and Approval Process for Repair/Maintenance/Alterations Fabricator/Construction Contractor prepares repair/maintenance/alterations WP complying with Saudi Aramco Welding Engineering Standards and submits it to Proponent
Engineering/Maintenance Div. receives the WP and screens if it need CSD formal approval as per Table 1?
No
Yes Fabricator/Construction Contractor receive and review CSD comments and correct WP deficiencies
WP rejected
CSD welding specialist/engineer reviews WP
Engineering/Maintenance Div. receives WP review Results WP accepted
WP rejected
Proponent Inspection Unit reviews and approves the application of WP WP accepted Engineering/Maintenance Div. formally accepts the WP and sends the approval to Fabricator/Construction Contractor
Fabricator/Construction Contractor can use the welding procedure
Page 14 of 14
View more...
Comments